Nanocrystalline Core rau Inverter
Siv nanocrystalline core rau ib hom hom inductor muaj qhov zoo ntawm cov khoom siv xws li ferrite, feem ntau vim nws cov khoom sib nqus zoo dua.
Nanocrystalline High-Frequency Inverter Core muaj ntau yam kev siv hauv kev siv hluav taws xob hluav taws xob vim nws cov khoom siv hluav taws xob zoo heev. Cov ntawv thov tshwj xeeb yog raws li hauv qab no:
Siab -Cov khoom siv hluav taws xob ntau zaus
- PFC Inductors: Hauv AC/DC thiab DC/DC converters, nanocrystalline cores yog tshwj xeeb tshaj yog haum rau pem hauv ntej - kawg PFC inductors. Lawv tuaj yeem txo qhov siab - zaus poob thiab txhim kho lub zog.
- Main Transformers: Nanocrystalline cores tuaj yeem siv rau hauv cov transformers loj. Lawv siab - saturation sib nqus induction thiab qis - poob yam ntxwv tso cai rau kev tsim ntawm me me - ntim transformers tsis muaj saturation, yog li txhim kho efficiency.
- Cov zis lim inductors: Thaum siv nyob rau hauv cov zis lim inductors, nanocrystalline cores tuaj yeem txhim kho cov yam ntxwv ripple, ua rau kev ua haujlwm ruaj khov ntawm cov khoom siv hluav taws xob.
Tshiab Zog Fais Fab Tsim Tshuab
- Photovoltaic Inverters: Hauv photovoltaic inverters, kev siv nanocrystalline cores hauv boost inductors tuaj yeem txo qhov poob ntau dua 20%. Ntxiv mus, qhov ntim me me ntawm siab - zaus rho tawm transformers ua los ntawm nanocrystalline cores yog qhov tsim nyog rau kev sib koom ua ke, thiab lawv qhov dav - qhov kub thiab txias tuaj yeem hloov mus rau qhov chaw sab nraum zoov hnyav.
- Cua zog Converters: Zoo ib yam li photovoltaic inverters, nanocrystalline cores hauv cov tshuab hluav taws xob cua tshuab kuj tuaj yeem ua lub luag haujlwm hauv kev txo qhov poob thiab pab txhawb cov khoom siv miniaturization, txhim kho tag nrho cov txiaj ntsig thiab kev ntseeg siab ntawm lub cev.
Electric Tsheb Fais Fab Systems
- Ntawm - Board Chargers (OBC): Nanocrystalline cores tuaj yeem txhim kho qhov ua tau zoo ntawm - board chargers, yog li txuas ntxiv kev tsav tsheb ntawm hluav taws xob. Nyob rau tib lub sijhawm, lawv daim ntawv thov kuj tuaj yeem pab txhawb rau qhov miniaturization ntawm OBCs, txuag tsheb sab hauv qhov chaw.
- DC / DC Converters: Hauv lub tsheb hluav taws xob DC / DC converters, nanocrystalline cores tuaj yeem txo qhov ntim thiab qhov hnyav ntawm cov converters, txhim kho kev ua haujlwm, thiab ua kom zoo dua qhov kev ua tau zoo ntawm tag nrho lub tsheb lub zog.
- Tsav Tsav Inverters: Nanocrystalline cores tuaj yeem siv rau hauv cov khoom lim dej ntawm cov tsav lub cev muaj zog inverters los ua kom zoo lim dej, txo cov electromagnetic cuam tshuam, thiab txhim kho kev ruaj ntseg thiab kev ua haujlwm ntawm lub tshuab tsav.
Industrial Inverters
- Tso zis lim Reactors: Hauv kev lag luam inverters, kev siv cov ntaub ntawv nanocrystalline hauv cov zis lim reactors tuaj yeem txo qis kev sib raug zoo, txhim kho qhov zoo ntawm cov zis tam sim no, thiab txo qhov cuam tshuam ntawm daim phiaj hluav taws xob.
- Siab - zaus Pulse Transformers: Nanocrystalline cores muaj kev ua haujlwm ruaj khov nyob rau hauv siab - zaus pulse transformers, uas tuaj yeem ua kom muaj kev ua haujlwm zoo ntawm kev lag luam inverters nyob rau hauv siab - zaus thiab siab - fais fab tej yam kev mob thiab txo cov khoom tsis ua hauj lwm.
Tsis tas li ntawd, nanocrystalline siab - zaus inverter cores kuj siv rau hauv inverter vuam tshuab, X - ray tshuab, laser fais fab mov, UPS fais fab mov, thiab lwm yam khoom siv.
Tsawg-Hwj chim siab-Frequency Inverter Magnetic Core
|
TSIS MUAJ. |
Nano core specification |
Kev ua tau zoo (20KHz, 0.5T) |
Lwm yam kev ua tau zoo |
|
1 |
ONL-64 * 40 * 20 |
P <28W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 60μH |
|
2 |
ONL-80 * 50 * 20 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 60μH |
|
3 |
ONL-80 * 50 * 20 |
P <30W/Kg, Br ≤0.28T |
|
|
4 |
ONL-80 * 50 * 25 |
P <30W/Kg, Br ≤0.28T |
|
|
5 |
Loj: 90 * 40 * 20 |
--- |
G Ntau dua lossis sib npaug rau 0.52Kg, U Ntau dua lossis sib npaug rau 50V |
|
6 |
ONL-100 * 50 * 25 |
--- |
G Ntau dua lossis sib npaug rau 0.76Kg, U Ntau dua lossis sib npaug rau 60V |
|
7 |
ONL-155 * 95 * 55 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 167μH |
|
8 |
ONL-50 * 32 * 20 |
P <28W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 57μH |
|
9 |
ONL-50 * 32 * 20 |
P <28W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 57μH |
|
10 |
ONL-50 * 32 * 20 |
P <28W/Kg, Br ≤0.28T |
1KHz, 0.3V Al{2}} ~ 50μH |
|
11 |
ONL-50 * 32 * 20 |
P <28W/Kg, Br ≤0.28T |
1KHz, 0.3V Al{2}} ~ 48μH |
|
12 |
ONL-50 * 32 * 20 |
P <28W/Kg, Br ≤0.28T |
1KHz, 0.3V Al{2}} ~ 60μH |
|
13 |
ONL-50 * 32 * 20 |
P <28W/Kg, Br ≤0.28T |
1KHz, 0.3V Al{2}} ~ 50μH |
|
14 |
ONL-50 * 32 * 20 |
P <28W/Kg, Br ≤0.28T |
1KHz, 0.3V Al{2}} ~ 43μH |
|
15 |
ONL-55 * 37 * 30 |
P <30W/Kg, Br ≤0.28T |
|
|
16 |
ONL-64 * 40 * 20 |
P <28W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 60μH |
|
17 |
ONL-64 * 40 * 20 |
P<28W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 60μH |
|
18 |
ONL-64 * 40 * 20 |
P<28W/Kg, Br ≤0.28T |
1KHz, 0.3V Al{2}} ~ 60μH |
|
19 |
ONL-64 * 40 * 20 |
P<28W/Kg, Br ≤0.28T |
|
|
20 |
ONL-64 * 40 * 35 |
P <30W/Kg, Br ≤0.28T |
|
|
21 |
ONL-70 * 40 * 20 |
P <28W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 71μH |
|
22 |
ONL-70 * 40 * 20 |
P <28W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 71μH |
|
23 |
Loj: 70 * 40 * 25 |
P <28W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 84μH |
|
24 |
Loj: 70 * 40 * 25 |
P <28W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 84μH |
|
25 |
Loj: 70 * 40 * 25 |
P <28W/Kg, Br ≤0.28T |
1KHz, 1V Al=60-90μH |
|
26 |
Loj: 70 * 40 * 25 |
P <30W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 84μH |
|
27 |
Loj: 70 * 40 * 25 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 84μH |
|
28 |
Loj: 70 * 40 * 25 |
P <30W/Kg, Br ≤0.28T |
1KHz, 0.3V Al{2}} ~ 60μH |
|
29 |
ONL-80 * 50 * 20 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 60μH |
|
30 |
ONL-80 * 50 * 20 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 60μH |
|
31 |
ONL-80 * 50 * 20 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 60μH |
|
32 |
ONL-80 * 50 * 25 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug li 75μH |
|
33 |
ONL-80 * 50 * 25 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug li 75μH |
|
34 |
ONL-80 * 50 * 25 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug li 75μH |
|
35 |
ONL-80 * 50 * 25 |
P <30W/Kg,Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug li 75μH |
|
36 |
ONL-80 * 50 * 25 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug li 75μH |
|
37 |
ONL-80 * 50 * 25 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug li 75μH |
|
38 |
ONL-80 * 50 * 25 |
P <30W/Kg, Br ≤0.28T |
U>12V |
|
39 |
ONL-80 * 50 * 25 |
P <30W/Kg, Br ≤0.28T |
U>15V |
|
40 |
ONL-80 * 50 * 25 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug li 75μH |
|
41 |
ONL-80 * 50 * 25 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug li 75μH |
|
42 |
ONL-80 * 50 * 25 |
P <30W/Kg, Br ≤0.28T |
1KHz, 0.3V Al{2}} ~ 70μH |
|
43 |
ONL-100 * 60 * 20 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 65μH |
|
44 |
ONL-100 * 60 * 20 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 65μH |
|
45 |
ONL-100 * 60 * 20 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 65μH |
|
46 |
ONL-100 * 60 * 20 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 65μH |
|
47 |
ONL-100 * 60 * 20 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 65μH |
|
48 |
ONL-100 * 60 * 20 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 65μH |
|
49 |
ONL-100 * 60 * 20 |
P <30W/Kg, Br ≤0.28T |
U>12V |
|
50 |
ONL-100 * 60 * 20 |
P <30W/Kg, Br ≤0.28T |
U>15V |
|
51 |
ONL-100 * 60 * 20 |
P <30W/Kg, Br ≤0.28T |
1KHz, 0.3V Al{2}} ~ 65μH |
|
52 |
ONL-100 * 50 * 25 |
10KHz 0.5T, P<9W/Kg, Br ≤0.2 |
10KHz, 1V Al=62-110μH |
|
53 |
ONL-100 * 50 * 25 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 108μH |
|
54 |
ONL-100 * 50 * 25 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 108μH |
|
55 |
ONL-120 * 60 * 30 |
P <30W/Kg, Br ≤0.28T |
U=118V,I<300mA |
|
56 |
ONL-120 * 60 * 30 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 130μH |
|
57 |
ONL-120 * 60 * 30 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 130μH |
|
58 |
ONL-120 * 60 * 30 |
P <30W/Kg, Br ≤0.28T |
20KHz, 1V Al=77 ~ 90μH |
|
59 |
ONL-120 * 60 * 30 |
P <30W/Kg, Br ≤0.28T |
U>25V |
|
60 |
ONL-120 * 60 * 30 |
P <30W/Kg, Br ≤0.28T |
U>30V |
|
61 |
ONL-120 * 70 * 20 |
P <30W/Kg, Br ≤0.28T |
U=118V,I<450mA |
|
62 |
ONL-120 * 70 * 20 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 69μH |
|
63 |
ONL-120 * 70 * 20 |
P <30W/Kg,Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 69μH |
|
64 |
ONL-120 * 70 * 20 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 69μH |
|
65 |
ONL-120 * 70 * 20 |
P <30W/Kg, Br ≤0.28T |
U>15V |
|
66 |
ONL-120 * 70 * 25 |
P <30W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 86μH |
|
67 |
ONL-120 * 70 * 25 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 86μH |
|
68 |
ONL-120 * 70 * 25 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 86μH |
|
69 |
ONL-120 * 70 * 25 |
P <30W/Kg, Br ≤0.28T |
|
|
70 |
ONL-120 * 70 * 30 |
P <30W/Kg, Br ≤0.28T |
U=118V,I<300mA |
|
71 |
ONL-120 * 70 * 30 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 103μH |
|
72 |
ONL-120 * 70 * 30 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 103μH |
|
73 |
ONL-120 * 70 * 30 |
P <30W/Kg, Br ≤0.28T |
20KHz, 1V Al=65 ~ 75μH |
|
74 |
ONL-120 * 70 * 30 |
P <30W/Kg, Br ≤0.28T |
20KHz, 1V Al{2}} ~ 83μH |
|
75 |
ONL-120 * 70 * 30 |
P <30W/Kg, Br ≤0.28T |
U>22V |
|
76 |
ONL-120 * 70 * 40 |
P <30W/Kg, Br ≤0.28T |
|
|
77 |
ONL-130 * 80 * 40 |
P <30W/Kg, Br ≤0.28T |
U=118V,I<300mA |
|
78 |
ONL-130 * 80 * 40 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 120μH |
|
79 |
ONL-130 * 80 * 40 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 120μH |
|
80 |
ONL-130 * 80 * 40 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al{2}} ~ 120μH |
|
81 |
ONL-130 * 80 * 40 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 120μH |
|
82 |
ONL-130 * 80 * 40 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 120μH |
|
83 |
ONL-130 * 80 * 40 |
P <30W/Kg, Br ≤0.28T |
U>25V |
|
84 |
ONL-130 * 80 * 40 |
P <30W/Kg, Br ≤0.28T |
20KHz, 1V Al{2}} ~ 85μH |
|
85 |
ONL-130 * 80 * 40 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 120μH |
|
86 |
ONL-130 * 80 * 50 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 150μH |
|
87 |
ONL-130 * 80 * 50 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 150μH |
|
88 |
ONL-130 * 80 * 50 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al=70 ~ 150μH |
|
89 |
ONL-130 * 80 * 50 |
P <30W/Kg, Br ≤0.28T |
U>25V |
|
90 |
ONL-130 * 80 * 50 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 150μH |
|
91 |
ONL-130 * 80 * 50 |
P <30W/Kg, Br ≤0.28T |
20KHz, 1V Al=78 ~ 90μH |
|
92 |
ONL-130 * 90 * 50 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 115μH |
|
93 |
ONL-130 * 90 * 50 |
P <30W/Kg,Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 115μH |
|
94 |
ONL-130 * 90 * 50 |
P <30W/Kg, Br ≤0.28T |
U>25V |
|
95 |
ONL-165 * 115 * 40 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 90μH |
|
96 |
ONL-165 * 115 * 50 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 113μH |
|
97 |
ONL-110 * 65 * 25 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 84μH |
|
98 |
ONL-110 * 65 * 30 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 100μH |
|
99 |
ONL-105 * 60 * 30 |
P <27W/Kg, Br ≤0.25T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 107μH |
|
100 |
ONL-105 * 60 * 30 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 107μH |
|
101 |
ONL-105 * 60 * 30 |
P <30W/Kg, Br ≤0.28T |
U>30V |
|
102 |
ONL-105 * 60 * 40 |
P <30W/Kg, Br ≤0.28T |
|
|
103 |
ONL-170 * 110 * 50 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 135μH |
|
104 |
ONL-290 * 210 * 50 |
P <35W/Kg,Br ≤0.30T |
1KHz, 1V Al Tsawg dua lossis sib npaug rau 101μH |
|
105 |
ONL-80 * 50 * 25 |
P <30W/Kg, Br ≤0.28T |
G Ntau dua lossis sib npaug rau 0.4Kg 1KHz, 1V Al Ntau dua lossis sib npaug rau 41μH |
|
106 |
ONL-100 * 60 * 20 |
P <30W/Kg, Br ≤0.28T |
G Ntau dua lossis sib npaug rau 0.52Kg 1KHz, 1V Al Ntau dua lossis sib npaug rau 36μH |
|
107 |
ONL-120 * 60 * 30 |
P <30W/Kg, Br ≤0.28T |
G Ntau dua lossis sib npaug rau 1.26Kg 1KHz, 1V Al Ntau dua lossis sib npaug rau 72μH |
|
108 |
ONL-120 * 70 * 25 |
P <30W/Kg, Br ≤0.28T |
G Ntau dua lossis sib npaug rau 0.94Kg 1KHz, 1V Al Ntau dua lossis sib npaug rau 47μH |
|
109 |
ONL-130 * 80 * 40 |
P <30W/Kg, Br ≤0.28T |
G Ntau dua lossis sib npaug rau 1.6Kg 1KHz, 1V Al Ntau dua lossis sib npaug rau 64μH |
|
110 |
ONL-70 * 40 * 20 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
111 |
ONL-70 * 40 * 20 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
112 |
Loj: 70 * 40 * 25 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
113 |
Loj: 70 * 40 * 25 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
114 |
ONL-80 * 50 * 20 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
115 |
ONL-80 * 50 * 20 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
116 |
ONL-80 * 50 * 25 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
117 |
ONL-80 * 50 * 25 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
118 |
ONL-80 * 50 * 30 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
119 |
ONL-100 * 60 * 20 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
120 |
ONL-100 * 50 * 25 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
121 |
ONL-100 * 50 * 25 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
122 |
ONL-105 * 60 * 30 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
123 |
ONL-120 * 60 * 30 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
124 |
ONL-120 * 70 * 20 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
125 |
ONL-120 * 70 * 25 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
126 |
ONL-120 * 70 * 30 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
127 |
ONL-130 * 80 * 40 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
128 |
ONL-130 * 80 * 50 |
P Tsawg dua lossis sib npaug rau 33W / Kg, Br Tsawg dua lossis sib npaug rau 0.33T |
|
|
129 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
130 |
ONL-64 * 40 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
131 |
ONL-64 * 40 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
132 |
ONL-70 * 40 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
133 |
ONL-70 * 40 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
134 |
Loj: 70 * 40 * 25 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
135 |
Loj: 70 * 40 * 25 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
136 |
ONL-80 * 50 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
137 |
ONL-80 * 50 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
138 |
ONL-80 * 50 * 25 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
139 |
ONL-80 * 50 * 25 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
140 |
ONL-80 * 50 * 30 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
141 |
ONL-100 * 60 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
142 |
ONL-100 * 50 * 25 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
143 |
ONL-100 * 50 * 25 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
144 |
ONL-105 * 60 * 30 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
145 |
ONL-120 * 60 * 30 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
146 |
ONL-120 * 70 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
147 |
ONL-120 * 70 * 25 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
148 |
ONL-120 * 70 * 30 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
149 |
ONL-130 * 80 * 40 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
150 |
ONL-130 * 80 * 50 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
|
|
151 |
ONL-50 * 32 * 20 |
P <30W/Kg, Br ≤0.28T |
1 KHz, 0.25V L>24mH@22Ts(AL>50μH) |
|
152 |
ONL-50 * 32 * 20 |
P <30W/Kg, Br ≤0.28T |
1KHz,1V Al≤60μH,Q>15 |
|
153 |
ONL-50 * 32 * 20 |
P <30W/Kg, Br ≤0.28T |
1KHz, 0.3V Al{2}} ~ 40μH |
|
154 |
ONL-50 * 32 * 20 |
P <30W/Kg, Br ≤0.28T |
1 KHz, 0.3V L=20-30mH@21TS(Al{2}}~68μ H) |
|
155 |
ONL-50 * 32 * 20 |
P <30W/Kg, |
1KHz, 0.25V Al{2}} ~ 60μH |
|
156 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
1KHz, 0.3V Al{2}} ~ 60μH |
|
157 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
1KHz, 0.3V Al{2}} ~ 50μH |
|
158 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
1KHz,0.3V Al>60μH |
|
159 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
1KHz, 0.3V Al{2}} ~ 60μH |
|
160 |
ONL-50 * 32 * 20 |
P <30W/Kg, Br ≤0.28T |
1KHz, 1V Al=35 ~ 55μH |
|
161 |
ONL-50 * 32 * 20 |
实测(P <30W/Kg, Br ≤ 0.28T) |
1KHz, 0.3V Al Ntau dua lossis sib npaug rau 50μH |
|
162 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 20W / Kg, Br Tsawg dua lossis sib npaug rau 0.20T |
-- |
|
163 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 20W / Kg, Br Tsawg dua lossis sib npaug rau 0.20T |
1KHz, 0.3V Al{2}} ~ 40μH |
|
164 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 20W / Kg, Br Tsawg dua lossis sib npaug rau 0.20T |
1KHz, 0.3V Al Ntau dua lossis sib npaug rau 45μH |
|
165 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 20W / Kg, Br Tsawg dua lossis sib npaug rau 0.20T |
1KHz, 0.3V Al{2}} ~ 60μH |
|
166 |
ONL-50 * 32 * 20 |
P<30W/Kg, Br <0.28T |
1KHz, 0.3V Al{2}} ~ 45μH |
|
167 |
ONL-50 * 32 * 20 |
P<30W/Kg, Br <0.28T |
1KHz, 0.3V Al{2}} ~ 54μH |
|
168 |
ONL-50 * 32 * 20 |
P<30W/Kg, Br <0.28T |
1KHz, 1V Al-40μH |
|
169 |
ONL-50 * 32 * 20 |
P<30W/Kg, Br <0.28T |
1KHz, 1V Al=40 ~ 50μH |
|
170 |
ONL-50 * 32 * 20 |
P<30W/Kg, Br <0.28T |
1KHz, 1V Al=50 ~ 60μH |
|
171 |
ONL-50 * 32 * 20 |
P<30W/Kg, Br <0.28T |
1KHz, 1V Al60μH |
|
172 |
ONL-50 * 32 * 20 |
P<30W/Kg, Br <0.28T |
1KHz, 1V Al=40 ~ 70μH |
|
173 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 20W / Kg, Br Tsawg dua lossis sib npaug rau 0.20T |
1KHz, 0.3V Al{2}} ~ 50μH |
|
174 |
ONL-50 * 32 * 20 |
P<30W/Kg, Br <0.28T |
1KHz, 0.3V Al-40μH |
|
175 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
1KHz, 0.3V, AL=40-60μH |
|
176 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
1KHz, 1V Al=25-57μH |
|
177 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
1KHz 0.25V, Al=34-55μH |
|
178 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
1KHz 0.25V, Al Ntau dua lossis sib npaug rau 50μH |
|
179 |
ONL-50 * 32 * 20 |
P Tsawg dua lossis sib npaug rau 30W / Kg, Br Tsawg dua lossis sib npaug rau 0.28T |
1KHz 0.3V, Al=30-60μH |
Lwm qhov loj me thiab kev ua tau zoo tuaj yeem kho tau.

Peb lub Hoobkas
Sunbow Group tshwj xeeb hauv kev tsim, kev tsim kho thiab tsim tawm tshiab -hom amorphous, nanocrystalline, silicon steel nplooj ntawv thiab lwm yam khoom sib nqus thiab cov khoom muaj feem xyuam. Tam sim no, lub tuam txhab muaj ob lub hauv paus tsim nyob rau hauv Anhui thiab Zhejiang, nrog rau ntau cov patented technologies, thiab tau dhau ISO9001, IATF16949 zoo tswj system ntawv pov thawj.Tag nrho cov khoom tau dhau ROHS, SGS thiab lwm yam kev tiv thaiv ib puag ncig certification.
Lub tuam txhab muaj cov cuab yeej siv siab heev xws li loj- nplai lub tshuab nqus tsev smelting furnaces, lub zog txau siv, ntau yam sib nqus annealing furnaces thiab kev koom tes nrog cov tsev kawm tshawb fawb hauv tsev thiab cov tsev kawm qib siab, uas ua kom lub tuam txhab R & D muaj peev xwm thiab cov khoom zoo. Lub tuam txhab cov khoom tseem ceeb suav nrog ntau hom amorphous, nanocrystalline strips thiab siab thiab qis voltage tam sim no transformer cores, precision tam sim no transformer cores, hom hom inductor cores, PFC inductor cores, siab zaus fais fab transformer cores thiab lwm yam khoom siv. Nws tsuas yog ua haujlwm ntawm lub zog tshiab, lub zog hluav taws xob photovoltaic, tsim hluav taws xob cua, cov khoom siv hauv tsev ntse, cov ntsuas ntse, wireless charging, thiab ntau yam khoom siv hluav taws xob, inverters, lim inductors, thiab cov ntaub ntawv tiv thaiv hauv lub teb chaws txoj kev lag luam tawm tshiab.







Peb qhov kev sim
|
Lub npe |
Ntau zaus thiab tam sim no ntau yam |
Xeem lub hom phiaj |
|
Mos sib nqus AC / DC tester |
AC: 0-100KHZ lossis DC AC: 0-100KHZ lossis DC |
Txhawm rau ntsuas qhov tsis sib xws ntawm cov khoom sib nqus ntawm cov khoom sib nqus AC / DC tam sim no |
|
Mos magnetic poob tester |
0-500KHZ 0-500KHZ |
Txhawm rau kuaj qhov poob ntawm cov khoom sib nqus mos |
|
LCR tester |
20HZ-30MHZ (MAX) 20HZ-30MHZ (MAX) |
Txhawm rau ntsuas qhov inductance, tsis kam thiab capacitance |
|
Pulse coil tester |
Lub hwj chim: 0-3000V |
Interturn withstand voltage test, poob xeem thiab inductance sib txawv xeem |
|
Withstanding voltage tester |
Lub hwj chim: 0-5000V |
Kev ntsuas hluav taws xob tiv thaiv |
|
Rwb thaiv tsev tiv thaiv tester |
100MΩ |
Rwb thaiv tsev tsis kam |
|
DC superposition tester |
Zaus: 20HZ-1MHZ Tam sim no: 0-40A |
DC superimposed inductor |
|
Pulse DC superposition tester |
Tam sim no: 0-1000A |
DC superimposed inductor |
|
Siab- zog peb-theem reactor kuaj lub rooj zaum |
Tam sim no: 0-2000A (MAX) |
Peb-phase inductance test, peb-theem siab tam sim no ntsuas kub nce siab, ntsuas kev sib haum xeeb |















Cov ntawv pov thawj

Peb cov txheej txheem ntau lawm

FAQ
Q: Koj puas yog tuam txhab lag luam lossis chaw tsim khoom?
A: Peb yog cov chaw tsim khoom tshwj xeeb hauv kev tsim, kev tsim kho thiab tsim tawm tshiab -hom amorphous, nanocrystalline, silicon steel nplooj ntawv thiab lwm yam khoom sib nqus thiab cov khoom siv.
Q: Koj lub peev xwm ntau lawm yog dab tsi?
A: Lub peev xwm tsim tau txhua xyoo ntawm amorphous & nanocrystalline ribbon yog 600 tons;
Lub peev xwm tsim khoom txhua xyoo ntawm lub zog hluav taws xob cov tub ntxhais yog 35 lab;
C- hom hlau core txhua xyoo muaj peev xwm ntawm 240 tons;
Txhua xyoo muaj peev xwm ntawm reactors yog 50,000;
Lub peev xwm tsim txhua xyoo ntawm precision transformers yog 40 lab;
Q: Koj puas tuaj yeem ua OEM thiab ODM?
A: Yog, OEM thiab ODM yog ob qho tib si txais. Cov khoom siv, xim, style tuaj yeem hloov kho, qhov yooj yim kom muaj nuj nqis peb yuav qhia tom qab peb sib tham.
Q: Koj puas tuaj yeem tsim raws li peb qhov kev xav tau?
A: Yog, Peb muaj ib pab neeg ua haujlwm uas muaj kev paub dhau los hauv kev tsim kho.
Sunbow muab ntau yam sib nqus cores ua los ntawm amorphous ribbons thiab nanocrystalline ribbons.
Nanocrystalline Cores:
Cores rau tam sim no Transformers
Cores rau Cov Hluav Taws Xob Hluav Taws Xob
Cores rau Switched Hom Fais Fab
Nanocrystalline C-Cores
Nanocrystalline Circular Cut Cores
Nanocrystalline Hom Hom Choke Cores
Precision Tam sim no Transformer Cores
Amorphous Cores:
Amorphous stator cores rau Electric Motors
Cores rau High Power Transformers
Cores rau nruab nrab zaus Transformers
PFC Choke Cores
Rectangular Txiav Cores
Cim npe nrov: nanocrystalline core rau inverter, Tuam Tshoj nanocrystalline core rau inverter manufacturers, lwm tus neeg, Hoobkas
Xa kev nug